The LE-7 rocket engine main injector has undergone a few occurrences of welded joint structural failure because it is subjected to high thermal stress during the engine start and stop sequence. The low-cycle fatigue test and high-strain fatigue test which were conducted as part of failure analysis revealed that the welded joint has a considerably shorter fatigue life than expected. To improve the ductility and toughness of the welded joint, high-temperature-solution heat treatment was applied after welding. The low-cycle fatigue life of a welded joint subjected to this solution heat treatment became three times longer than that without it. A design criterion was established for low-cycle fatigue life estimation, and the life requirement was found to be satisfied.